Would someone please share some recipes to make MoS2 solution usable in spin coater from solid powder form of MoS2. How can I make just a few layered MoS2 on my device?
Hello, i have the same problem can you please tell me how you prepared the solution of the MoS2 and how we can deposited the exfoliation of MoS2 in water? thank you
It is better to use NMP as an exfoliating agent. Actually MoS2 has very low solubilty in any solvent so it can be only dispersed. Mix MoS2 in NMP and sonicate it for few hours then centrifuge the solution. The supernatant can be used for spin coating.