I need to know the particle size for the test, concentration of acid, amount of sample to be tested and the apparatus to be used as well as how to analyze the solution.
3. Take 100 mL of Aqua Regia in a beaker and add 1 g of Ore to it. Heat the slurry over a hot-plate till you get a clear solution. During heating, there might be some loss in the volume of the solution. keep adding aqua regia to maintain the volume level at 100 mL.
4. The concentration of Iron in the solution can be determined by analytical Instrument like AAS, ICP-OES/ ICP-AES.
5. From the concentration value you can back calculate the iron content in ores.